浏览全部资源
扫码关注微信
1. 中国科学院 长春光学精密机械与物理研究所,吉林 长春,中国,130033
2. 中国科学院激发态物理重点实验室,吉林 长春,130033
收稿日期:2001-08-16,
修回日期:2002-01-28,
纸质出版日期:2002-07-20
移动端阅览
张海明, 王之建, 张立功, 元金山. CdS纳米粒子的自组装单分子膜制备研究[J]. 发光学报, 2002,23(4): 369-372
ZHANG Hai-ming, WANG Zhi-jian, ZHANG Li-gong, YUAN Jin-shan. Synthesis, Study of CdS Nanoparticles by Self-assembled Monolayer[J]. Chinese Journal of Luminescence, 2002,23(4): 369-372
利用巯基乙酸与草酸的混合自组装单分子膜成功制备了粒径分布均匀的CdS纳米粒子
并用SEM
XRD
XPS
PL对样品进行了表征.SEM表明形成在自组装单分子膜表面上的CdS纳米粒子的平均粒径约为45nm.XPS表明在自组装单分子膜表面形成了CdS纳米粒子.PL谱表明CdS纳米粒子在675nm有一峰值波长
我们认为这一发光是由表面缺陷造成的.
In the past decade
preparation of nanoparticles whose sizes and size distribution can be well controlled has become an important subject in materials science fields. Many methods have been developed in preparation of semiconductor nanoparticles
such as Langmuir-Blodgett (LB) films
colloid-chemical
electrochemical
electrophoresis
thermolysis of organometallic compounds in solution
template and self-assembled monolayers etc. The self-assembled monolayer was reported by Sagtiv in 1983. Hereafter the method has attracted wide interesting due to its simple operation
easy preparation
and no need of complex instruments
but it meets great difficulties to obtain a desirable size distribution.A new method for preparation of nearly monodisperse CdS nanoparticles by self-assembled monolayers of mercaptoacetic acid and oxalic acid is reported. The mercaptoacetic acid plays an important role in the formation of the CdS nanoparticles. The preparation procedures were shown in Fig. 1. There include three major steps:First
preparing of self-assembled monolayers of mercaptoacetic acid and oxalic acid on aluminum substrate; Second
immersing the substrate into solution containing Cd
2+
to exchange ions; Third
Cd
2+
reaction with H
2
S gas to form CdS nanoparticles. In the formation process of the nanoparticles
CdS molecular formed at mercaptoacetic acid will play a role of nuclear center. The CdS nanoparticles were characterized by SEM
XRD
XPS and PL
respectively. SEM image indicates that the average size is about 45nm
which is well agreement with XRD result. Room temperature PL spectrum shows that CdS has a wide emission band in the range from 500 to 800nm about and the emission peak is at 675nm
which is attributed to surface defects.
0
浏览量
101
下载量
1
CSCD
关联资源
相关文章
相关作者
相关机构